Ferralium 255 (UNS S32550, also written F61) is the one super duplex grade that carries 1.5–2.5% copper. That addition does not raise PREN much — it sits around 40, close to 2507 — but it changes how the alloy behaves under flowing, particle-laden fluid. In sand-producing wells it is the difference between choke trim that lasts a campaign and trim that is pulled twice a year.

The copper addition lowers the corrosion potential slightly and promotes a more tenacious passive film under abrasion, which is why the grade is specified for valve trim, pump internals and flow measurement hardware in erosive service. Straight 2507 is stronger in pure pitting terms but loses material faster when sand is present.
Mechanically it sits with the super duplex family: 550 MPa minimum yield, 760 MPa tensile, and a ferrite-austenite balance that gives roughly twice the fatigue strength of austenitic stainless. It machines more readily than 2507 at comparable hardness, which matters for choke bevels and threaded connections.
The limits are the same as other duplex grades — no long-term service above about 300 °C, a 32 HRC ceiling under NACE MR0175, and a sharp toughness transition at low temperature. Where those bind, the answer is a nickel alloy, not a duplex variant.
Ferralium 255 Standards and Equivalent Grades
Bar and forging stock are supplied to A479 and A182 F61 respectively; plate is A240 and pipe A790. In the European system the grade is 1.4507 (X2CrNiMoCuN25-6-3). It should not be confused with F55 / S32760 (Zeron 100), which also contains copper and tungsten but has a different composition and a higher PREN.
| System | Designation |
| UNS | S32550 |
| W.Nr. / EN | 1.4507 / X2CrNiMoCuN25-6-3 |
| ASTM A479 / A276 | Bar for machining |
| ASTM A182 F61 | Forging, flange, valve part |
| ASTM A240 | Plate, sheet and strip |
| ASTM A790 | Seamless and welded pipe |
Where Ferralium 255 Is Used
Choke trim and bevels
Positive and adjustable choke internals in sand-producing wells, where erosion rather than corrosion sets the replacement interval.
Pump casings and impellers
Multiphase and produced water pumps handling solids, resistant to erosion-corrosion at the cutwater and impeller eye.
Valve balls, seats and stems
Ball valve internals for slurry and produced sand service, where galling and erosion occur together.
Orifice plates and flow meters
Metering elements downstream of sand screens, where sharp edges must survive without rounding over.
Wear rings and bushings
Sleeve bearings and wear rings in seawater-lubricated pumps, avoiding the galvanic couple of a bronze against stainless.
Agitators and mixer shafts
Produced water and drilling fluid tanks, where abrasion and chloride attack combine.
Supply Range and Condition
Round bar from 16 mm to 350 mm diameter, peeled, turned or ground; open-die forged blocks from 100 mm to 600 mm section; near-net valve and choke bodies to drawing. Standard condition is solution annealed at 1,040–1,120 °C, water quenched, pickled or machined.
Testing includes chemistry with copper and nitrogen reported per heat, tensile and hardness across the section, ferrite content by metallography (target 40–60%), ASTM A923 Method A and C, and ASTM G48 Method A pitting test where specified. EN 10204 3.1 certificates as standard.
Chemical Composition of Ferralium 255 (wt%)
Copper at 1.50–2.50% is the defining element and must be reported on the certificate; a heat without it is a 2507 substitute, not Ferralium 255. Nitrogen at 0.10–0.25% keeps the weld zone balanced and contributes to the yield strength.
| Element | Min % | Max % |
| Chromium (Cr) | 24.00 | 27.00 |
| Nickel (Ni) | 4.50 | 6.50 |
| Molybdenum (Mo) | 2.90 | 3.90 |
| Copper (Cu) | 1.50 | 2.50 |
| Nitrogen (N) | 0.10 | 0.25 |
| Carbon (C) | — | 0.040 |
| Manganese (Mn) | — | 1.50 |
| Silicon (Si) | — | 1.00 |
| Phosphorus (P) | — | 0.040 |
| Sulphur (S) | — | 0.030 |
| Iron (Fe) | balance | balance |
Mechanical Properties of Ferralium 255 Bar
Values are typical minima for solution-annealed bar at room temperature. As with all duplex grades, hardness is capped at 32 HRC for NACE MR0175 sour service and must be checked on the finished part.
| Property (room temperature) | Typical minimum |
| Tensile strength | ≥ 760 MPa |
| Yield strength (0.2%) | ≥ 550 MPa |
| Elongation in 50 mm | ≥ 15% |
| Hardness (NACE limit) | ≤ 32 HRC |
Need Ferralium 255 bar or choke trim stock?
Send the diameter or drawing, quantity, condition and any erosion or NACE requirement — we reply with mill availability, lead time and a priced offer, usually within one working day.