TWZ-4 is TISCO’s molybdenum-nickel non-magnetic grade: 965 MPa minimum yield in HS temper, 1.7–2.5% molybdenum and 3.0–4.5% nickel for pitting resistance in heavy sections, relative permeability 1.005 max, to works specification Q/TX 085-2019.

TWZ-4 is the molybdenum-nickel member of the TISCO non-magnetic family. It is not stronger than TWZ-3 in HS temper — both are guaranteed at 965 MPa — it is more corrosion resistant: 1.7 to 2.5 percent molybdenum and 3.0 to 4.5 percent nickel hold pitting resistance in heavy sections and in chloride-rich mud where the leaner grades run out of margin.
Grade and specification
| Item | TWZ-4 |
|---|---|
| Mill | TISCO (Taiyuan Iron & Steel) |
| Works specification | Q/TX 085-2019 |
| Type | Austenitic Mn-Cr-Mo-Ni-N, low carbon |
| Product forms | Forged bar, rolled bar, hollow bar, collar blanks |
| Temper | HS (cold worked) or LS (solution annealed) |
The designation is the mill’s. It is what appears on the mill test certificate and on the shipping documents — we do not re-badge grades.
Applications
Non-magnetic drill collars and BHA components in wells where pitting, not load, sets the service life.
- Heavy-section collars where cold reduction is limited by the bar size
- Wells with high chloride mud or elevated bottom-hole temperature
- MWD and LWD housings that must hold permeability through machining
- Stabiliser mandrels and non-magnetic subs in corrosive service
- Replacement for nickel-based alloys where an austenitic Mn-Cr-Mo-N grade will do the duty
Sizes and delivery
| Form | Range |
|---|---|
| Forged / rolled round bar | OD 80 – 300 mm |
| Hollow bar and collar blanks | OD 90 – 280 mm, bore to drawing |
| Cut-to-length | Any length up to 6 m |
| HS temper | Guaranteed up to OD 280 mm, banded |
| Custom melt | 3 – 5 t minimum for a fresh induction melt |
Chemical composition
Heat analysis, mass percent, to Q/TX 085-2019.
| Element | TWZ-4 | Element | TWZ-4 |
|---|---|---|---|
| C | max. 0.04 | Cr | 18.00 – 19.00 |
| Si | max. 1.00 | Mo | 1.70 – 2.50 |
| Mn | 20.00 – 23.50 | Ni | 3.00 – 4.50 |
| P | max. 0.025 | N | 0.55 – 0.70 |
| S | max. 0.010 | Nb, Ti, V | trace additions permitted |
Full limits are printed on the mill certificate; a specimen certificate is available before you order.
Mechanical properties
Minimum values at room temperature, by outside-diameter band.
| Property | HS temper, OD ≤ 235 mm | HS temper, OD 235–280 mm | LS temper, OD 80–450 mm |
|---|---|---|---|
| Yield strength Re, min. | 965 MPa | 900 MPa | 900 MPa |
| Tensile strength Rm, min. | 1035 MPa | 1035 MPa | 1035 MPa |
| Elongation A, min. | 20% | 20% | 20% |
| Impact KV, min. | 100 J | 100 J | 100 J |
| Hardness | 330–430 HBW, surface | 330–430 HBW, surface | 330–430 HBW, surface |
Relative permeability ≤ 1.005 and magnetic field gradient ≤ 0.05 µT per 100 mm, verified on every collar by probe testing and supplied as a printout with the certificate. 1 ksi = 6.895 MPa.
Melting and processing
- Melting: EAF + AOD, LF refining, then ingot or vertical casting; ESR on request
- Hot working: forged or rolled with a reduction ratio of 6 or better
- Heat treatment: solution anneal and water quench; warm forging followed by quenching to prevent sensitisation
- Finishing: peeled, turned, BTA bored, gun-drilled, thread and shoulder to drawing
Inspection and certification
- Chemical analysis and mechanical testing per heat to ASTM A370
- ASTM A262 Practice A and E for intergranular attack
- ASTM G36 / G38 C-ring stress-corrosion testing on request
- Full-length ultrasonic inspection to API Spec 7-1 clause 12
- Probe testing of permeability on every bar, printout supplied
- EN 10204 3.1 certificate as standard, 3.2 and SGS / TÜV on request
Need TWZ-4 non magnetic collar bars?
Send the outside diameter, bore, length, temper and quantity, plus any sour-service or permeability requirement — we reply with mill availability, certificate scope and a priced offer, usually within one working day.